Fiberglass Boat Osmosis Treatment

This procedure is useful in the following cases:

  • Presence of osmosis blisters on the hull — osmosis repair on fiberglass hulls
  • Absence of osmosis blisters — preventive osmosis protection on fiberglass hulls

Verification of osmosis on the boat

  • Winter storage / haul‑out
  • Perform a visual inspection of the hull: if blisters of various sizes are present, it is necessary to verify whether they are caused by osmosis. To check, simply pierce them with a cutter: if a viscous liquid with a vinegar‑like smell comes out, this indicates that the osmosis process has begun.

Support preparation — when no osmosis blisters are present

  • If no osmosis blisters are detected, proceed by removing the antifouling layers through sanding, scraping or a specific paint remover, bringing the hull back to gelcoat. If a paint remover is used, lightly sand the gelcoat with 80‑grit abrasive paper.
  • Measure the hull’s moisture content using a fiberglass moisture meter.
  • If the meter indicates no moisture, a preventive anti‑osmosis treatment can be applied. Before starting, rinse thoroughly with fresh water and allow to dry completely.

Preventive anti‑osmosis treatment

  • If holes, depressions or other discontinuities are present in the gelcoat, level them using EpoGryps OSMO PROOF epoxy resin thickened with THICKENING Additive (1–2% by weight). Once cured, sand with 80‑grit paper and remove dust with compressed air.
  • Apply at least 3 coats of EpoGryps OSMO PROOF by roller or brush (approx. 200 microns per coat). To achieve a smoother, more hydrodynamic surface, lightly sand with 150–180 grit and clean with compressed air between coats. If more than 24 hours pass between coats (at 20°C), sanding with 150–180 grit is required before applying the next coat.
  • Sand with 220–240 grit, remove dust with compressed air and apply the chosen antifouling system.

Support preparation — when osmosis blisters are present

  • If osmosis is active and blisters are present, in addition to removing the antifouling, the gelcoat must also be removed (via sandblasting, grinding or peeling).
  • Open, widen and clean the blisters (using hot water).
  • Measure the hull’s moisture content with a fiberglass moisture meter. Moisture is a prerequisite for osmosis activation.
  • Before the repair treatment, rinse thoroughly with fresh water (periodically, at least once a month) and allow the hull to dry completely until no moisture remains.
  • First, repair the laminate damage caused by osmosis (see the “Fiberglass repair” guide).

Osmosis repair treatment

  • Once all laminate irregularities caused by osmosis blisters have been filled and closed, sand with 80‑grit paper, remove dust with compressed air and apply one coat of EpoGryps OSMO PROOF epoxy resin by roller or brush to impregnate all open porosities.
  • If needed, within 24 hours (at 20°C), apply EpoGryps OSMO PROOF mixed with EVO THICKENING Additive (70–80% by weight). This mixture behaves like a filler and allows you to rebuild the removed gelcoat thickness. The first coat is applied with a notched trowel, with tooth height matching the required filler thickness (1.5–2 mm). Once cured, lightly sand with 80‑grit and clean with compressed air. The second coat, applied within 24 hours of the first (20°C), is applied with a smooth trowel to close the voids left by the first layer. Once cured, lightly sand with 80‑grit.
  • Proceed with at least 3 coats of EpoGryps OSMO PROOF by roller or brush (approx. 200 microns per coat). For a hydrodynamic surface, lightly sand with 150–180 grit and clean with compressed air between coats. If more than 24 hours pass between coats (20°C), sanding is required before the next application.
  • Sand with 220–240 grit, remove dust with compressed air and apply the chosen antifouling system.

Download the Work Sheet:
see procedure link

Osmosis repair on a fiberglass hull

Take a look at the various phases of the osmosis repair treatment on a fiberglass hull: from gelcoat removal and blister opening, to moisture measurement and hull drying, up to the application of EpoGryps OSMO PROOF and final antifouling.

BeforeAfter